Heat resistant conveyor belt temperature grade selection goes wrong in a predictable way. A buyer measures the material at the kiln discharge, reads 150 °C, asks for a "150-degree belt," and receives a belt whose cover survives the temperature and whose carcass does not. Six months later the belt is stiff, the top cover has a fine crazing across it, the splice has opened, and the supplier points to the datasheet that said 150 °C. Everyone was right and the belt still failed.

The reason is that "heat resistance" is three different questions folded into one number: what temperature the cover compound tolerates, what temperature the carcass fabric tolerates, and what temperature the belt actually reaches in service, which is neither the material temperature nor the ambient. This article separates the three, explains what the T-grades and ISO classes mean, and sets out what to specify and what evidence to demand from a belting works before you commit to a hot-duty belt.

What the grades mean and where they come from

Two designation systems cover heat-resistant textile belting and most Chinese quotations use one or the other, sometimes both on the same sheet.

DIN 22102-3 grades the cover compound by the maximum material temperature the belt is designed to run under, using T followed by a temperature: T120, T150 and T180 are the common steps, with some makers offering T200 and above under their own names. The number is nominally the continuous conveyed-material temperature the cover is rated for, with a higher short-term peak allowed.

ISO 4195 classifies heat resistance by test rather than by duty, with classes T1, T2 and T3 defined by ageing the cover in a hot-air oven at a stated temperature for a stated period and measuring how much the compound changed in hardness, tensile strength and elongation. Roughly, T1 corresponds to light duty, T2 to medium, T3 to the hottest service, and each class sits at a higher oven temperature than the last.

The two are not interchangeable and a quotation that lists "T150 / T2" is making an equivalence the standards do not make. Treat the T-grade as the supplier's statement of intended duty and the ISO class as the thing a laboratory can test. Read the current editions of both before you write either into a purchase order — the tests, the ageing periods and the acceptance limits are what your inspection will be measured against, not the number in the belt name.

Designation Approximate intended duty What it does not tell you
T120 (DIN 22102-3) Material up to about 120 °C continuous, higher short peaks Carcass type, peak duration allowed, what happens above the limit
T150 (DIN 22102-3) Material up to about 150 °C continuous Whether the carcass is standard EP or heat-stabilised
T180 (DIN 22102-3) Material up to about 180 °C continuous Compound base (EPDM or otherwise) unless separately stated
ISO 4195 class T1 / T2 / T3 Cover compound aged in hot air at increasing oven temperatures and held within stated property-change limits Anything about the conveyed material or the carcass — it is a cover test
Supplier's own "T200" / "T250" No published basis; check against ISO 4195 test at the stated temperature Everything unless a laboratory report is supplied

The three temperatures that matter

A cement plant with clinker at 150 °C at the loading point is the classic case, and it illustrates why one number is not enough.

Material temperature is what you measured. It is the input, not the belt condition.

Belt surface temperature is what the top cover reaches. It depends on the material temperature, the lump size, the depth of the load, the belt speed and the length of the run. Fine hot material — clinker dust, sinter fines, foundry sand — makes intimate contact with the cover and transfers heat fast; large lumps touch the belt at a few points and transfer far less. A belt under 150 °C clinker fines can run hotter at the cover surface than one under 200 °C lumps. Contact time matters too: a slow belt with a deep bed heats through, a fast belt with a shallow bed does not.

Carcass temperature is what the fabric reaches, and it is the one that kills belts. The top cover insulates the carcass; a thicker top cover on a hot-duty belt is not extra wear allowance, it is thermal insulation, and a heat belt ordered with a thin top cover to save money will cook its fabric. Polyester, the E in EP fabric, loses strength and shrinks at temperatures well below what the cover compound tolerates; nylon is a little better in some respects and worse in others. Once the carcass has been heat-shrunk it never returns, the belt gets shorter and stiffer, and the splice, which was made at a different length, is the first thing to let go.

The practical consequence: the grade you ask for should be chosen on the belt surface temperature you expect, with the carcass type and top cover gauge chosen on the carcass temperature you can tolerate. If you have not calculated or measured belt temperature, you are guessing, and a supplier is guessing with you.

Compound and carcass choices by duty

Heat resistance in the cover comes from the base polymer and the cure system, not from a coating. The broad hierarchy used across the trade:

  • SBR-based compounds with heat-stabilising additives cover the T120 band. Cheapest, and the compound most Chinese works run by default when a buyer says "heat resistant" without a number.
  • Blended or chlorobutyl-based compounds reach the T150 band in some formulations.
  • EPDM-based compounds are the usual basis for T150 to T180 and above. EPDM resists heat ageing and ozone well and is the compound to expect in any belt sold for genuinely hot duty. It is also more expensive and, in most formulations, less abrasion-resistant than a good SBR — which is the trade-off a clinker line lives with. The earlier piece on cover rubber abrasion grades covers why the two properties pull against each other.

On the carcass side:

  • Standard EP fabric is fine for T120 duty with adequate top cover.
  • Heat-stabilised or heat-set EP fabric is offered by some works for T150 duty; ask what the treatment is and for evidence it was applied.
  • Aramid carcasses hold strength at temperatures that destroy polyester, weigh less, and cost a great deal more. They are the answer for T180 and above where belt life, not first cost, is the number that matters.
  • Heat-resistant skim compound between the plies matters as much as the cover. A hot belt that delaminates between plies while the cover looks fine has usually been built with a standard skim under a heat-resistant cover — a common cost-cut and impossible to see from outside. Ask for the skim compound to be stated on the construction sheet.

A note on how carcass strength is quoted: the ply rating and total belt strength should be read from the EP ply and tension rating guide rather than assumed from the number of plies, because a heat belt often needs a stronger carcass than the load alone would justify, to give margin for the strength the fabric will lose in service.

The signs a heat belt is failing, and what they mean

Someone who has walked a clinker conveyor for a few years reads the belt like a chart. These are the symptoms and their usual causes.

Fine cracking across the top cover, worse at the loading zone. Cover compound has hardened from heat ageing. If the belt is young, the compound was under-rated for the surface temperature; if it is old, this is normal end of life. Measure hardness with a Shore A durometer at the loading point and at the return side and compare — a large spread says the cover is being cooked in one place.

Belt has shortened and take-up is running out of travel. Carcass shrinkage, almost always polyester. The cover may look perfect. This is the failure a T-grade on the cover will not prevent, and the one an aramid or heat-set carcass exists to stop.

Top cover blistering or bubbling. Volatiles or moisture in the material flashing to steam under the belt surface, or the cover-to-carcass adhesion failing under heat. Either way the belt was not built for the duty.

Splice opens first. The splice compound and adhesion were not rated for the belt temperature, or the splice was made on a belt that has since shrunk. Ask for the splice materials to carry the same heat rating as the belt, and get that in writing, because it is the item most likely to be substituted.

Bottom cover cracking. The return run is not cooling the belt. Hot belts rely on the return run to shed heat; a short conveyor with a long loaded section and a short return runs hotter than the same belt on a long conveyor. If you cannot lengthen the return, consider a cooler cover grade one step up.

Specifying and verifying: an inspection checklist

A heat belt that meets its specification is verified in three places: on paper before the order, on the roll before shipment, and on the line after commissioning.

Before the order — on paper

  1. State the material, its temperature at the loading point, lump size distribution, moisture and the belt speed and loaded length. Ask the supplier to state the belt surface temperature they have designed for.
  2. State the grade in both systems — the T-grade you want and the ISO 4195 class you will test against — and say which governs if they disagree.
  3. State top and bottom cover gauge separately; for hot duty the top cover carries the insulation duty and should be thicker than the bottom.
  4. State the carcass fabric type and whether it is heat-stabilised, the skim compound, and the total belt strength.
  5. Ask whether the supplier holds hot-air ageing test data to ISO 188 on the actual compound, and at what temperature and for how long. A works that mixes its own compound can produce this; a works that buys compound in from the cluster should be able to obtain it from its compounder. Either answer is acceptable; "no data" is not.
  6. Ask for the splice kit or hot-vulcanising materials to be specified to the same heat grade.

Before shipment — on the roll

  1. Have the cover hardness, cover gauge and ply construction checked against the construction sheet, and cut a sample from the roll end, not from a separate sample press. A third-party pre-shipment inspection can do this in an afternoon if you give the inspector the construction sheet and the test methods.
  2. Send the cut sample for an ISO 4195 ageing test at a laboratory you choose, if the belt carries a duty where a failure stops the plant. The cost is small against the belt.

After commissioning — on the line

  1. Record belt surface temperature at the loading zone and at the tail after the first week of full-rate running, with an infrared thermometer.
  2. Record belt length and take-up position at commissioning and monthly for the first quarter. Shrinkage shows here before it shows anywhere else.
  3. Record Shore A hardness at three points on the top cover at commissioning and quarterly.

Common questions

Is a T150 belt overkill for material at 120 °C?

Sometimes it is the right call. If the material is fine, the bed is deep, the belt is slow and the return run is short, the belt surface may run close to the material temperature and the carcass will run hotter than a T120 construction assumes. Grade on the belt temperature, not the material temperature, and when you do not know the belt temperature, one grade of margin is cheaper than one early replacement.

Can a heat belt also be abrasion-resistant?

Within limits. EPDM heat compounds generally give up abrasion resistance relative to a good SBR, and a supplier offering "T180 and top abrasion grade" in the same cover should be asked for both test results on the same compound. Where abrasion is severe and heat is moderate, a thicker top cover of a T120 or T150 compound often outlasts a thin cover of a hotter grade.

Does the ISO 4195 class prove the belt will survive my line?

No. It proves the cover compound holds its properties in a hot-air oven for the test period. It says nothing about the carcass, the skim, the splice, or the belt temperature your line produces. It is a necessary check, not a sufficient one.

What does a heat-resistant belt cost relative to a standard belt?

Ask for both quoted on the same construction sheet. The premium depends heavily on whether the compound is SBR-based or EPDM-based and whether the carcass is standard or aramid, so a blanket percentage would mislead more than it helps.

What to ask the supplier next

For any works quoting a hot-duty belt, the following go in the inquiry and the answers go in the contract. If the supplier is one you have not bought from before, read the guide on reading a Chinese certificate of conformity first, because most of what you receive back will be a document, and documents are where hot-duty claims go soft.

  • Which heat-resistant grades do you produce, and what continuous and peak material temperature is each rated to? Ask for the compound base to be named.
  • Do you offer a heat-stabilised or aramid carcass, and at what total belt strength?
  • Is the skim compound between plies heat-rated to match the cover? Have it stated on the construction sheet.
  • Do you have ISO 188 hot-air ageing data on the compound you would use for my belt — from your own laboratory or your compounder's — and can you send the report with the issuing body, holder name and date visible?
  • Is the sample you send cut from a production press batch?
  • What splice materials ship with the belt, and are they rated to the same grade?
  • Which shipped orders for hot-duty belting can you reference, with destination and application?

Jiutong Conveyor Belting, a rubber belting works registered in 2024 in Boye County, Baoding, lists multi-ply fabric conveyor belting with compound grade specified per order and directs buyers to confirm any heat-resistant grade at inquiry; its stated terms of one-piece MOQ and custom samples in around ten working days suit a trial cut before a production roll. Which heat grades it runs and what ageing data sits behind them are not on its factory profile, so those are the first questions to ask, and any test report that comes back should be read for issuing body, holder name and validity date before it is read for the number.